The W/m·K on the sheet belongs to the dielectric. Worked through for a 1 W LED, each step up buys fewer degrees.
The thermal conductivity printed on an aluminum-base laminate, 1.0, 2.0 or 8.0 W/m·K, is the conductivity of the dielectric layer alone. The aluminum underneath conducts around 200 W/m·K and the copper foil around 390 W/m·K (general material values), so the thin dielectric between them limits the heat flow, and what matters at the component is that layer's thermal resistance.
The formula: thermal resistance of the dielectric
A flat dielectric layer has a thermal resistance equal to its thickness divided by conductivity times area:
R = t / (k · A)
R in K/W, t = thickness in m, k = W/m·K, A = area in m²
Datasheets often give the area-independent form instead, R·A = t / k, in °C·cm²/W. A 100 µm dielectric at 1.0 W/m·K is 1.0 °C·cm²/W; at 2.0 W/m·K it is 0.5 °C·cm²/W. Temperature rise across the layer is ΔT = P · R.
Worked case: a 1 W LED soldered to a 3 × 3 mm thermal pad (A = 9 mm² = 9 × 10−6 m²) on a 100 µm dielectric, with heat assumed to pass straight down through the pad area only.
k = 2.0: R = 100 × 10−6 / (2.0 × 9 × 10−6) = 5.56 K/W → ΔT = 5.56 °C at 1 W
| Grade (W/m·K) | R·A (°C·cm²/W) | R (K/W) | ΔT at 1 W (°C) | Gain over grade below (°C) |
|---|---|---|---|---|
| 1.0 | 1.00 | 11.11 | 11.1 | – |
| 1.5 | 0.67 | 7.41 | 7.4 | 3.7 |
| 2.0 | 0.50 | 5.56 | 5.6 | 1.9 |
| 3.0 | 0.33 | 3.70 | 3.7 | 1.9 |
| 5.0 | 0.20 | 2.22 | 2.2 | 1.5 |
| 8.0 | 0.13 | 1.39 | 1.4 | 0.8 |
Resistance falls as 1/k, so each step up buys fewer degrees. Going from 1.0 to 2.0 W/m·K removes 5.6 °C; going from 5.0 to 8.0 removes 0.8 °C.
Copper spreading shrinks the gap between grades
Copper foil carries heat sideways before it enters the dielectric, so under a small pad the real dielectric resistance is lower than the one-dimensional figure, and lower by more on the low grades.
A rough fin estimate for 1 oz (35 µm) copper gives a spreading length of about √(kCu · tCu · t / k): 1.2 mm per side at 1.0 W/m·K and 0.4 mm at 8.0 W/m·K. The effective square grows to about 5.3 mm and 3.8 mm, and the dielectric resistance becomes roughly:
1.0 W/m·K: 3.5 K/W · 2.0: 2.3 K/W · 3.0: 1.8 K/W · 8.0: 0.85 K/W
A less conductive dielectric pushes heat further along the copper, which is why spreading cuts the 1.0 grade by about two thirds and the 8.0 grade by about 40 %. On this pad the step from 2.0 to 8.0 W/m·K is worth about 1.5 °C at 1 W, against 4.2 °C in the table.
Dielectric thickness counts as much as the grade
Resistance is proportional to thickness, so halving the dielectric does what doubling the grade does. Same 3 × 3 mm pad, no spreading:
- 50 µm at 1.0 W/m·K
- 5.56 K/W
- 100 µm at 2.0 W/m·K
- 5.56 K/W
- 150 µm at 3.0 W/m·K
- 5.56 K/W
- 75 µm at 2.0 W/m·K
- 4.17 K/W
A thinner layer also breaks down at a lower voltage, so thickness is usually fixed by the insulation requirement first and the grade chosen after; the numbers for that are in dielectric thickness and breakdown voltage. Compare grades at the same thickness, or compare R·A.
The rest of the stack decides whether the grade matters
Between an LED junction and the heatsink, the dielectric is one resistance in series with the package, solder, foil, base and interface, and for a 1 W LED the package is usually the largest. Junction-to-solder-point figures on 1 W package datasheets commonly fall somewhere between 3 and 10 K/W. The other layers, as general values over 9 mm²:
- Solder, 50 µm at about 50 W/m·K: 0.11 K/W, more with voids.
- Copper foil, 35 µm: 0.01 K/W.
- Aluminum base plus the interface to the heatsink: taken here as 0.5 K/W after spreading; the real figure depends on base thickness, flatness and interface material.
With an 8 K/W package and the spreading figures above, junction to heatsink totals about 12.1 K/W on a 1.0 W/m·K dielectric, 10.9 K/W on 2.0 and 9.5 K/W on 8.0. Moving from 2.0 to 8.0 W/m·K buys about 1.5 °C at 1 W. The heatsink-to-air resistance after all of this is often larger still.
How to pick a grade from this
A higher grade pays when the dielectric is a large share of the junction-to-heatsink resistance, which happens with high heat flux or a package below about 1 K/W. As a starting point:
- 1.0 to 2.0 W/m·K for about 1 W per 9 mm² pad or less with a package of 5 K/W or more. The dielectric is a minor term.
- 3.0 W/m·K when the dielectric must stay thick for voltage, or the flux reaches several W per 10 mm². It brings a 150 µm layer back to the resistance of 100 µm at 2.0.
- 5.0 to 8.0 W/m·K, or a copper base for packages near or below 1 K/W, such as chip-on-board LEDs and power semiconductors. At 10 W on a 5 × 5 mm pad through 100 µm, the dielectric rise without spreading is 20 °C at 2.0 W/m·K and 5.0 °C at 8.0.
Between these, test two grades on the real layout and measure junction temperature. Grade, base, copper weight and size can be set in the selector, where samples of both are requested. Sheets from different sources are only comparable when the conductivity was measured the same way; see reading an IMS laminate datasheet.